Pitting on packaging frames in washdown areas is usually a chloride problem, not a "stainless isn't stainless" problem. A quick first screen is the pitting resistance equivalent number, PREN = %Cr + 3.3 × %Mo + 16 × %N. Typical ranges are about 18–20 for 304, about 23–28 for 316, and about 35 for duplex 2205. Higher means more resistance to chloride pitting at a given temperature and chloride level.
PREN is a ranking tool, not a design rule. Crevices under bolted brackets, guards, and gaskets, stagnant films that dry and concentrate chloride, and chlorinated sanitizers at elevated temperature can all pit a grade that looks fine on paper. Design details (open frames, sealed tube ends, sloped surfaces, no lap joints) often do more than an alloy upgrade. What do you run on frames that see daily chlorinated washdown?
Poll: What's on your washdown-area machine frames?